참고 물성표
|
Tenacity |
Modulus |
Elonga-tion |
Density |
Moisture Regain |
LOI |
Heat Resistance* |
|
cN/dtex |
GPa |
cN/dtex |
GPa |
% |
g/cm3 |
% |
|
C |
| Zylon® AS |
37 |
5.8 |
1150 |
180 |
3.5 |
1.54 |
2.0 |
68 |
650 |
| Zylon® HM |
37 |
5.8 |
1720 |
270 |
2.5 |
1.56 |
0.6 |
68 |
650 |
| p-Aramid(HM) |
19 |
2.8 |
850 |
109 |
2.4 |
1.45 |
4.5 |
29 |
550 |
| m-Aramid |
4.5 |
0.65 |
140 |
17 |
22 |
1.38 |
4.5 |
29 |
400 |
| Steel Fiber |
3.5 |
2.8 |
290 |
200 |
1.4 |
7.8 |
0 |
|
|
| HS-PE |
35 |
3.5 |
1300 |
110 |
3.5 |
0.97 |
0 |
16.5 |
150 |
| PBI |
2.7 |
0.4 |
45 |
5.6 |
30 |
1.4 |
15 |
41 |
550 |
| Polyester |
8 |
1.1 |
125 |
15 |
25 |
1.38 |
0.4 |
17 |
260 |
*Melting or Decomposition Temperature
고온고습환경 강도변화 (180도씨50시간 처리후)